Material for sample of bitumen











              Compaction Machine                                                  Water Bath

             4.0     DETAILED PROCEDURE :

                                                                                       REFERENCE
                                      WORK PROCESS                                    DOCUMENT
             The procedure of this test is stated in detail BS 1377:1985


             A.   Preparation of Specimen (Premix)
              1. Aggregates and fillers that will be used are be determined

              2. The mixture comprises sufficient aggregate, sand and filler to
                  produce a specimen of  approximately 1200g. Preheat the

                  aggregate in oven at 150 C for at least 4 hours
              3. Heat the bitumen at the same temperature or the temperature of

                  the mixture

              4. The hot aggregate, will be heated again in bowl (pan). Heat
                  without adding any  bitumen mix for 1-2 minutes. Then add the
                  correct amount of bitumen. The bitumen  content that is used is the
                  percentage of weight of the total mix. Use bitumen content ... %

              5. The temperature during the mixing of aggregate and bituminous
                  mixture should not  be below than 137 C

              6. While preparing the mixture, the ram and Marshall mold should be
                  cleaned and  heated to 137 C

              7. Put the mold on the table and put a piece of filter paper into the

                  mold. Pour the hot  mix into the mold and smoothen the top
                  surface. Then put another piece of filter  paper.